Edge banding closes the raw edge of a board with edge tape, so the edge keeps moisture out, stands up to knocks and looks like the face of the board. The usual choice is plastic tape, ABS or PVC: thin on the front edges of the carcass and, most often, 2 mm on all four edges of the fronts. Edges against the wall, under the worktop and at the back need no tape, unless they are near water.

What edge tape does, and the types you can buy

Academy lesson 6.1Edge banding typesWatch the lesson →

Edge tape does three jobs. It seals the edge, because an open edge of melamine-faced particleboard (MFC, chipboard) takes in moisture and swells. It protects the edge from knocks, because the edge is softer than the face. And it gives the edge the same look as the face, in the same decor.

There are four kinds:

TypeWhat it isGood forFinishing
ABSplastic in a colour or decor, often textured; tough, no chlorinefronts, carcasses, edges that take knockstrimmed and rounded after gluing
PVCplastic in a colour or decor; flexible, but contains chlorinethe same as ABStrimmed and rounded after gluing
Melaminepaper soaked in melamine resin; thin and stiff, cracks easilyhidden edges, shelves, repairsoften pre-glued, applied with an iron
Veneera thin sheet of real wood, the back often reinforced with fleeceveneered boardssanded, then lacquered, oiled or waxed with the board

Plastic tapes have a primer on the back that the glue grips better. For fronts and edges that take knocks they are a better choice than melamine.

Four rolls of edge tape on a turntable: two plastic, one thin melamine and one veneer
From the left: white plastic tape, plastic tape in a wood decor, thin melamine edging and oak veneer edging.

Edge banding thickness and width

Edge tape runs from thin 0.4 mm up to 2 mm and more. Which thicknesses come in which decor is in the tape manufacturer’s catalogue. One rule decides it: thin tape where a front covers the edge, thicker tape where the edge is touched and knocked.

Thicker tape can also be rounded, so the edge doesn’t feel sharp under your hand. Thin tape stays almost sharp, and knocks show on it sooner.

Two door samples close up: on the left thin edge tape with an almost sharp arris, on the right thick edge tape with a rounded one
Left, 0.4 mm tape, almost sharp; right, 2 mm tape, rounded.

Edge tape is always a little wider than the board is thick, so it covers the whole edge, and the excess is trimmed off afterwards. For an 18 mm board that is, for example, tape 23 mm wide, and for a 38 mm worktop 43 mm.

Tape is sold in rolls and paid for by the metre. You order it by decor, width and thickness, pre-glued (for an iron) or without glue (for a machine). When you add up the metres from a cutting list, allow extra for trimming the ends, because tape is always cut with an overhang.

Which edges to band: carcass, fronts and open shelves

Academy lesson 6.2Which edge and how thickWatch the lesson →

Edge tape goes on the edges that are seen and touched. Look at a cabinet from where people look at it. A base unit is seen from above and from the front, a wall unit from below. So the bottom of a wall unit is easy to forget: the front edge of the bottom panel and the lower edges of the sides or the bottom, depending on the construction.

The carcass gets tape on the front edges of the side panels, the bottom, the cross rails and the shelves. With the doors closed the front covers them, so thin tape is enough. Where there is no front, as with open shelves and the end side panel of a run, the carcass edge is on show like a front, so it often gets the same tape as the fronts.

Fronts get tape on all four edges, most often 2 mm, because doors and drawers are touched and knocked every day. All the edges of one front have the same thickness, so it looks the same all round.

PartEdges with tapeTape by the rule of the tradeEFS default (on all four edges)
Side panels, bottom, cross rails (behind a front)front edgesthin0.4 mm
Shelves and dividersfront edgethin0.4 mm
Open shelves, end side panel of a runthe edges on showoften the same as the fronts0.4 mm, change by hand
Doors, flaps, drawer frontsall four edgesmost often 2 mm, the same all round2 mm
Sink unit: bottom and side panelsevery edge, hidden ones tooalways banded0.4 mm
Side panels by a floor that gets moppedthe lower edges toobanded even when not seen0.4 mm
Worktopvisible; back edge against the wall without tape (bead or upstand)tape 43 mm wide for a 38 mm worktop2 mm, wall edge included
Kickboard and fillersvisible; filler edge against the wall without tape–2 mm, wall edge included
Back panelnone–no edge tape
The Edging Tape box in EFS: Longer 1 set to 1 mm, Shorter 1, Longer 2 and Shorter 2 set to 2 mm
Tape is set for each of the four edges: two longer and two shorter.

Edges against the wall, under the worktop and near water

Edges that aren’t seen need no tape: the back edges against the wall, the top edges of the side panels under the worktop, and the edge of a filler that butts against the wall. The back edge of the worktop gets no tape either, but it is sealed with a bead or an upstand.

Some workshops band hidden edges too, with thin tape, for neatness and against moisture. That is their choice, but then the tape has to be in the cutting list too.

The exception is edges near water. In the sink unit, band every edge of the bottom and the side panels, even the ones nobody looks at, because that is exactly where water drips. The same goes for the lower edges of side panels next to a floor that gets mopped.

A section through a sink unit: the edges of the bottom and of the side panel next to the siphon and the dishwasher are picked out in blue
In the sink unit every edge of the bottom and the side panels gets tape, even the hidden ones.

A moisture-resistant board doesn’t change that: it copes with moisture better, but it is not waterproof, so its edges still get tape or sealant. More in Moisture-resistant cabinets.

Every banded edge changes the cut size. Without pre-milling, a part is cut smaller by the tape thickness on each banded edge: a door with a finished size of 716 × 396 mm and 2 mm tape all round is cut at 712 × 392 mm. How a cutting list works this out, with and without pre-milling, is shown in A cutting list for your panel supplier.

Glue: EVA, PUR and laser edging with a zero joint

Academy lesson 6.3Glues and machinesWatch the lesson →

Edge tape is glued with hot-melt glue. The glue is melted by heat and spread on the edge, and the joint holds as soon as it cools. So the tape holds only as well as the glue underneath it.

GlueStrengthWeakness
EVAthe most common, easy to work withsoftens again when warm, so copes less well with steam and heat
PURkeeps curing with moisture from the air and never softens again; copes better with water and heat; thinner glue lineneeds more care: glue left in the machine cures, so the machine is cleaned as its instructions say
Laser edgingno separate glue: a layer on the back is melted by a laser or another heat source; almost invisible joint (zero joint)needs special tape and a machine that can apply it

Next to a dishwasher or an oven, years of steam and heat can lift tape on EVA glue, while on PUR it stays put. That is why PUR is often chosen for kitchens and bathrooms. Glue comes in natural, white or clear, so you pick it to suit the decor.

Three white edges with edge tape close up: on the left a visible darker glue line, in the middle a thinner one, on the right almost none
The glue line on a white decor: EVA on the left, PUR in the middle, laser edging on the right.

Edge banding by hand with an iron, or with an edge bander

Without a machine you use pre-glued tape:

  1. Lay the tape on the edge, with a small overhang at both ends.
  2. An iron heats the tape until the glue melts. Right behind the iron, press the tape down with a wooden block and hold it until it cools.
  3. Once cool, cut off the ends, and trim the overhang along the faces with a knife or a hand edge trimmer.
  4. Lightly ease the arrises with fine sandpaper, without scratching the face.

Thin tapes, melamine or thin plastic, are the easiest to apply by hand. For thick tape and curved edges there are handheld edge banders, which heat the glue and apply it themselves.

Banding by hand: an orange glow of heat on the tape along the edge of a white shelf, with a wooden block following it
The heat (orange) melts the glue on the tape, and the wooden block right behind it presses the tape onto the edge.

An edge bander does all of this in one pass. The board travels along the conveyor past units that work in order: pre-milling, glue application, pressure rollers, end trimming, overhang trimming (straight or with a radius), scraping and buffing.

Pre-milling comes first: two cutters take a thin layer off the edge, because a sawn edge may have small chips, and a fresh, straight edge gives a thinner glue line. That allowance depends on the machine and goes on the cut size, so agree on it with whoever does the banding. By default EFS assumes that pre-milling takes off exactly the tape thickness, so the cut size equals the finished size. If the edge bander has no pre-milling unit, switch that off in the export settings (Cutting list and cut size).

An edge bander is set up for each thickness of tape and board, following the machine manufacturer’s instructions. Learn to work at it with someone who knows how.

Common edge banding mistakes

Bad banding is the first thing anyone notices, because it is on the edge everybody touches. These four come up most often (lesson 6.4):

  • A visible glue line. A dark line shows between tape and board, clearest on a light decor. The causes are too much glue, glue that is too cold, weak pressure or an uneven edge. A straight, clean edge, glue in the colour of the decor and a well set machine help, and PUR and laser edging give the thinnest line.
  • Tape coming off, most often at corners and ends. If the glue stays on the tape and the board underneath is almost clean, the glue never gripped. The causes are a cold board or workshop (a cold board cools the glue too soon), too little glue, a dusty or damp edge, and EVA next to steam and heat. So boards and tape stand in a warm workshop first, and the glue runs at the temperature on its data sheet.
  • Tape shorter than the edge. The bare corner takes in moisture and is the first to chip. Tape is always cut with an overhang at both ends, and the ends are trimmed only after gluing.
  • Tape out of line, or too narrow. A step is left on one side and part of the edge is bare on the other. Watch the overhang trimming too: tape left above the face makes a sharp edge that catches, and a cutter that bites too deep scratches the face.

Before a batch, run a test piece and check the glue line, the corners, the ends and the alignment. Whatever shows on the first piece would show on every one. More mistakes you can catch before cutting are in The most common custom cabinet mistakes.

Frequently asked questions

ABS vs PVC edge banding: what is the difference?

They look and work much the same: both are plastic, in a colour or decor, and are trimmed and rounded after gluing. ABS is tough and contains no chlorine. PVC is flexible but contains chlorine, so ABS is often chosen because it is easier to dispose of.

How thick should edge banding be on doors and on the carcass?

Fronts most often get 2 mm on all four edges, and the carcass gets thin tape on its front edges, because the front covers them. In EFS the default is 0.4 mm for the carcass and 2 mm for the fronts.

Can you apply edge banding with an iron?

Yes, with pre-glued tape. The iron heats the tape, and a wooden block right behind it presses the tape down until the glue cools. Thin tapes, melamine or thin plastic, are the easiest to do this way.

How do you edge band a worktop?

The tape is a little wider than the worktop is thick: for a 38 mm worktop, for example, 43 mm. The back edge against the wall gets no tape, but it is sealed with a bead or an upstand. The sink cut-out is sealed before the sink goes in, because the core of the board is open at its edge. Worktop types, thicknesses and joints are covered in Kitchen worktops.